Published: July 6, 2026 Reading time: 14 min Fundamentals

Eutectic vs Eutectoid vs Peritectic Reactions: Complete Comparison

Invariant reactions govern how phases nucleate, disappear, and rearrange at fixed temperature and composition points on any binary phase diagram. Eutectic, eutectoid, and peritectic reactions look superficially similar — three lines converging at a horizontal isotherm — but they involve fundamentally different parent and product phases, diffusion mechanics, and resulting microstructures. This guide compares all three side by side using the iron-carbon system as the working example, and includes an interactive lever rule calculator for computing phase fractions at each reaction.

Key Takeaways

  • A eutectic reaction converts one liquid into two solid phases: L → α + β. In the Fe-C system this occurs at 4.3 wt% C and 1147 °C, forming ledeburite.
  • A eutectoid reaction converts one solid phase into two different solid phases: γ → α + β. In steel this occurs at 0.77 wt% C and 727 °C, forming pearlite.
  • A peritectic reaction combines a solid and a liquid into a single new solid: L + α → β. In the Fe-C system this occurs near 0.17 wt% C and 1495 °C.
  • Eutectic and eutectoid reactions are structurally analogous (one phase splits into two); the peritectic reaction is the odd one out (two phases merge into one).
  • The lever rule applies to the tie lines flanking all three reactions, letting you calculate relative phase amounts just above and just below the invariant temperature.
  • Peritectic reactions are the most diffusion-limited of the three because the new phase forms as an isolating shell, often leaving untransformed material even under slow cooling.

Invariant Reaction Lever Rule Calculator

Select a reaction, confirm or edit the flanking phase compositions, enter the alloy’s overall composition, and calculate relative phase fractions using the lever rule.

Three Invariant Reactions — Schematic Phase Fields EUTECTIC L alpha beta L to alpha + beta EUTECTOID gamma alpha Fe3C gamma to alpha + Fe3C PERITECTIC delta L gamma L + delta to gamma Reading the shapes Eutectic and eutectoid: a single phase field (V shape) sits ABOVE the isotherm and splits into two phase fields below it. The difference is only whether the parent phase is liquid (eutectic) or solid (eutectoid). Peritectic: two DIFFERENT phase fields approach the isotherm from either side, above it, and merge into a single phase field below it — the reverse topology of eutectic/eutectoid.
Schematic comparison of the three invariant reaction topologies on a binary phase diagram. © metallurgyzone.com

What Is an Invariant Reaction?

An invariant reaction occurs at a fixed temperature and fixed phase compositions, with zero degrees of freedom under the Gibbs phase rule for a binary system at constant pressure (F = C − P + 1 = 2 − 3 + 1 = 0 when three phases coexist). Because F = 0, the reaction proceeds at constant temperature until one of the parent phases is fully consumed — it cannot occur over a temperature range the way ordinary solidification or solid-state transformations do. Eutectic, eutectoid, and peritectic reactions are the three most common invariant reactions encountered in binary metallic systems; monotectic, syntectic, and metatectic reactions exist but are far less common in structural alloys.

General forms (on cooling):
Eutectic:    L        →  α + β
Eutectoid:   γ (solid) →  α + β
Peritectic:  L + α    →  β

Eutectic Reactions

In a eutectic reaction, a single liquid phase decomposes on cooling into two solid phases simultaneously, at one fixed composition and temperature — the eutectic point. This is the lowest-melting composition in the system, which is why eutectic alloys (solder, cast iron, Al-Si casting alloys) are chosen where low, sharp melting points are advantageous.

Fe-C Eutectic: Ledeburite Formation

In the iron-iron carbide system, the eutectic reaction occurs at 4.3 wt% C and 1147 °C: liquid transforms into austenite (2.14 wt% C) plus cementite (6.67 wt% C). The resulting fine mixture is called ledeburite. This reaction is only relevant to cast irons and high-carbon alloys — plain carbon and low-alloy steels never reach 4.3 wt% C and therefore never pass through the eutectic point.

L (4.3% C) → γ (2.14% C) + Fe3C (6.67% C), at 1147 °C

Other Common Eutectic Systems

  • Pb-Sn solder: eutectic at 61.9 wt% Sn, 183 °C
  • Al-Si casting alloys: eutectic near 12.6 wt% Si, 577 °C
  • Ag-Cu: eutectic at 71.9 wt% Ag, 779.4 °C

Eutectoid Reactions

A eutectoid reaction has the identical topology as a eutectic reaction, but the parent phase is solid, not liquid. One solid phase decomposes into two different solid phases at a fixed composition and temperature.

Fe-C Eutectoid: Pearlite Formation

The eutectoid point in the Fe-C system sits at 0.77 wt% C and 727 °C. On slow cooling through this temperature, austenite transforms into pearlite — alternating lamellae of ferrite (0.022 wt% C) and cementite (6.67 wt% C). Pearlite is a microstructural constituent, not a phase; it consists of two distinct phases arranged in a characteristic lamellar morphology that nucleates at austenite grain boundaries and grows as coupled diffusion fronts.

γ (0.77% C) → α (0.022% C) + Fe3C (6.67% C), at 727 °C

This single reaction underpins essentially all conventional heat treatment of steel: annealing produces coarse pearlite, normalizing produces finer pearlite, and suppressing this reaction entirely by rapid quenching is what produces martensite instead.

Peritectic Reactions

A peritectic reaction is structurally the reverse of the other two: a solid phase and a liquid phase, present together above the reaction temperature, combine on cooling into a single new solid phase. Unlike eutectic and eutectoid reactions, the peritectic reaction consumes two parent phases to produce only one product phase.

Fe-C Peritectic: Delta to Austenite

The peritectic reaction in the Fe-C system occurs near 1495 °C, where delta-ferrite (about 0.09 wt% C) reacts with liquid (about 0.53 wt% C) to form austenite (about 0.17 wt% C). This reaction only affects steels solidifying with bulk composition in roughly the 0.09-0.53 wt% C range — most structural and machinery steels fall in this window during solidification, even though the reaction has no bearing on their room-temperature microstructure.

L (0.53% C) + δ (0.09% C) → γ (0.17% C), at 1495 °C

Why Peritectic Reactions Rarely Go to Completion

Because the new gamma phase nucleates at the delta-liquid interface, it forms as a shell that separates the two remaining parent phases. Further reaction requires solid-state diffusion through this shell, which is far slower than liquid-phase diffusion. Consequently, peritectic reactions are notoriously incomplete even under slow equilibrium cooling, and cored, non-equilibrium microstructures are common — a practical concern in continuous casting of peritectic-range steels, where it contributes to surface cracking.

Side-by-Side Comparison

FeatureEutecticEutectoidPeritectic
General equationL → α + βγ → α + βL + α → β
Parent phase(s)One liquidOne solidOne solid + one liquid
Product phase(s)Two solidsTwo solidsOne solid
Fe-C example temperature1147 °C727 °C~1495 °C
Fe-C example composition4.3 wt% C0.77 wt% C~0.17 wt% C
Fe-C product nameLedeburitePearliteAustenite (no special name)
Diagram shape above isothermSingle (liquid) fieldSingle (solid) fieldTwo different fields, either side
Diffusion characterLiquid-state, fastSolid-state, moderateSolid-state through product shell, slow
Typically reaches equilibrium?ReadilyReadily, given timeOften incomplete
Relevance to plain carbon steelCast irons only (>2% C)All hypo/hypereutectoid steelsLow-carbon steels during solidification only

Applying the Lever Rule at Each Reaction

Just below (or, for peritectic, just above) the invariant temperature, the alloy sits inside a two-phase field bounded by a horizontal tie line. The lever rule computes the mass fraction of each phase from the three compositions on that tie line — the same mechanics used anywhere on the iron-carbon phase diagram.

Fraction of left-side phase  W_left  = (C_right - C0) / (C_right - C_left)
Fraction of right-side phase W_right = (C0 - C_left) / (C_right - C_left)

Worked example (eutectoid steel, C0 = 0.77 wt% C):
  C_left  (ferrite)   = 0.022 wt% C
  C_right (cementite) = 6.67  wt% C
  W_ferrite   = (6.67 - 0.77) / (6.67 - 0.022) = 5.90 / 6.648 = 0.888  (88.8 wt%)
  W_cementite = (0.77 - 0.022) / (6.67 - 0.022) = 0.748 / 6.648 = 0.112  (11.2 wt%)

For the peritectic reaction, the same arithmetic determines whether delta-ferrite or liquid is present in excess relative to the exact peritectic ratio, which governs whether the alloy ends up fully austenitic or retains untransformed delta-ferrite just below 1495 °C. Use the calculator above with the “Peritectic” preset to run this for any composition in the 0.09-0.53 wt% C window.

Distinguishing the Reactions on an Unlabeled Diagram

Look at What Sits Above the Isotherm

If a single phase field sits directly above the horizontal invariant line and two different phase fields sit below it, the reaction is eutectic (if the single field above is liquid) or eutectoid (if it is solid). If two different phase fields approach the isotherm from opposite sides above it, converging into one phase field below, the reaction is peritectic.

Check the Number of Phases Consumed

Eutectic and eutectoid reactions consume one phase and produce two. Peritectic reactions consume two phases and produce one. This is the fastest diagnostic once you have identified the phase fields immediately above and below the isotherm.

Fe-Fe3C Diagram — Three Invariant Points (schematic, not to scale) Carbon content (wt% C, log-compressed for clarity) Temperature Peritectic: 1495 °C, ~0.17% C (L + δ → γ) liquidus Eutectic: 1147 °C, 4.3% C (L → γ + Fe3C) γ (austenite) Eutectoid: 727 °C, 0.77% C (γ → α + Fe3C) α (ferrite) 0.17% 0.77% 4.3%
Schematic Fe-Fe3C diagram (not to scale) locating the peritectic, eutectic, and eutectoid invariant points relative to one another. © metallurgyzone.com

Industrial Significance

Every plain carbon and low-alloy steel passes through the peritectic region during solidification if its composition falls below about 0.53 wt% C, then cools through the austenite field, and finally passes through the eutectoid point during any slow cool, anneal, or normalizing treatment. Cast irons additionally pass through the eutectic point during solidification. Understanding which reaction governs a given processing step is fundamental to controlling as-cast segregation, hot cracking susceptibility during continuous casting, and the final annealed or normalized microstructure. It also underlies interpretation of weld HAZ microstructures, where rapid thermal cycles can suppress or truncate the eutectoid reaction locally.

Frequently Asked Questions

What is the basic difference between a eutectic and a eutectoid reaction?
A eutectic reaction transforms a liquid directly into two solid phases on cooling (L → α + β), while a eutectoid reaction transforms one solid phase into two different solid phases (γ → α + β) with no liquid involved at any point.
What is a peritectic reaction and how does it differ from the other two?
A peritectic reaction combines a solid phase and a liquid phase on cooling to form a single new solid phase (L + α → β), whereas eutectic and eutectoid reactions each produce two product phases from one parent phase.
What is the eutectoid composition and temperature in the iron-carbon system?
The eutectoid point in the Fe-Fe3C system occurs at 0.77 wt% carbon and 727 °C, where austenite transforms into pearlite, a lamellar mixture of ferrite and cementite.
What is the eutectic composition and temperature in the iron-carbon system?
The eutectic point occurs at 4.3 wt% carbon and 1147 °C, where liquid transforms into austenite plus cementite, forming ledeburite. This reaction defines the melting behaviour of cast irons.
Where does the peritectic reaction occur in the iron-carbon system?
The peritectic reaction occurs at approximately 1495 °C, where delta-ferrite of about 0.09 wt% carbon reacts with liquid of about 0.53 wt% carbon to form austenite of about 0.17 wt% carbon. It affects only low-carbon steels solidifying near this composition range.
Is pearlite a phase or a microstructure?
Pearlite is not a phase. It is a two-phase microstructural constituent formed by the eutectoid reaction, consisting of alternating lamellae of ferrite and cementite.
Why are peritectic reactions harder to observe in practice than eutectic reactions?
Peritectic reactions are diffusion-limited because the new phase forms as a shell around the pre-existing solid, which slows further reaction. This often leaves untransformed primary phase behind even under near-equilibrium cooling, unlike eutectic reactions which proceed to completion more readily.
Can the lever rule be applied to all three invariant reactions?
Yes. The lever rule applies at any tie line in a two-phase region, including the tie lines that terminate at eutectic, eutectoid, and peritectic points, allowing calculation of relative phase amounts on either side of the invariant temperature.
What everyday alloy systems show eutectic behaviour besides steel?
Common eutectic systems include Pb-Sn solder near 61.9 wt% Sn at 183 °C, Al-Si casting alloys near 12.6 wt% Si at 577 °C, and Ag-Cu near 71.9 wt% Ag at 779.4 °C.
How can you identify an invariant reaction on a phase diagram at a glance?
Look at the shape formed by the boundary lines meeting at the horizontal invariant line. An upward-pointing V above the line with liquid at the apex indicates eutectic; a similar V entirely within the solid region indicates eutectoid; and an arrangement where a liquid and a solid approach from opposite sides above a horizontal line, meeting a single solid phase field below, indicates peritectic.

Recommended Reference Reading

ASM Handbook Vol. 3: Alloy Phase Diagrams

The definitive reference atlas covering binary and ternary phase diagrams, including detailed Fe-C invariant reaction data.

View on Amazon

Callister’s Materials Science and Engineering

Foundational textbook coverage of phase diagrams, the lever rule, and invariant reactions with worked problems.

View on Amazon

Physical Metallurgy Principles (Abbaschian/Abbaschian/Reed-Hill)

Rigorous treatment of phase transformations, diffusion-controlled reactions, and microstructural evolution in alloys.

View on Amazon

Steels: Microstructure and Properties (Bhadeshia and Honeycombe)

Advanced treatment of pearlite, bainite, and martensite formation building directly on the eutectoid reaction.

View on Amazon

Disclosure: MetallurgyZone participates in the Amazon Associates programme. If you purchase through these links, we may earn a small commission at no extra cost to you. This helps support free technical content on this site.

Further Reading

garg5917@gmail.com

← Previous
Binary Phase Diagrams: Reading Guide with Lever Rule and Worked Examples
Next →
Solidification of Metals: Nucleation, Dendrite Growth and Grain Structure