Quick answer t8/5 is the time a weld’s heat-affected zone takes to cool from 800 °C to 500 °C. EN 1011-2 gives two equations for C-Mn and low-alloy steels, a 3D one for thick plate and a 2D one for thin plate, and the valid result is the greater of the two. Enter your welding parameters below and the calculator does the rest.

How fast a weld cools through the 800–500 °C window decides whether the heat-affected zone (HAZ) stays tough or turns hard and crack-prone. This page gives you a calculator for that cooling time, the equations behind it, worked examples, and look-up tables computed from the same equations, so you can sanity-check a welding procedure before spending money on qualification tests.

t8/5 cooling time calculator

Valid for C-Mn and low-alloy steels. Auto mode compares the 2D and 3D results and reports the greater one.

Heat input
10 to 2000 A
5 to 100 V
mm per minute, not mm/s
Joint and plate
0 to 450 °C
1 to 300 mm

This is a design aid, not a substitute for a qualified welding procedure. Typical guidance for high-strength structural steels is about 5–25 s (see the section on target windows below), but your steel grade’s datasheet and procedure qualification govern.

What is t8/5 and why does 800–500 °C matter?

As a weld cools, the austenite in the HAZ decomposes into ferrite, pearlite, bainite or martensite. Ovako’s welding guide notes that the most crucial microstructural changes happen between 800 °C and 500 °C, which is why cooling is quoted as the time to cross that interval. It is the same continuous-cooling logic used for furnace heat treatment, explained in our guide to quenching steel, only applied to a weld thermal cycle.

The direction of the effect is straightforward. If heat input is low for the thickness and hardenability, fast cooling can make the HAZ fully martensitic, with high hardness and a high risk of cold cracking. Slower cooling gives softer, tougher products such as bainite or, in weld metal, acicular ferrite. Go too slow, though, and large grains reduce impact toughness. The wider picture of zones, hardness and cracking is in our article on the heat-affected zone in steel welds.

Schematic weld thermal cycle showing the t8/5 window Temperature rises rapidly to a peak near the fusion line, then falls. The time taken to fall from 800 degrees Celsius to 500 degrees Celsius is marked t8/5. Time Temperature 800 °C500 °C t8/5 Peak temperature near the fusion line
Schematic weld thermal cycle. The curve shape is illustrative, not plotted from data. t8/5 is the time between the two dashed temperature lines.

How is t8/5 calculated? The EN 1011-2 equations

For C-Mn and low-alloy steels, the cooling time can be calculated with the formulas in EN 1011-2 or read from cooling-time charts. There is one equation for thick plate, where heat flows away in three dimensions, and one for thin plate, where it is confined mainly to the plane of the plate:

3D (thick plate) t8/5 = (6700 − 5·T0) · Q · [1/(500 − T0) − 1/(800 − T0)] · F3 2D (thin plate) t8/5 = (4300 − 4.3·T0) · 10^5 · (Q/d)^2 · [1/(500 − T0)^2 − 1/(800 − T0)^2] · F2
Symbols and units
SymbolMeaningUnit
t8/5Cooling time from 800 to 500 °Cs
T0Working temperature: preheat, or interpass temperature for later runs°C
QEffective (net) heat inputkJ/mm
dPlate thickness (2D equation only)mm
F2, F3Joint shape factors for 2D and 3D flow–

The 3D result is proportional to heat input. The 2D result grows with the square of heat input and falls with the square of thickness, so doubling the thickness of a thin plate cuts its t8/5 to a quarter at the same heat input and preheat.

Step 1: net heat input

Arc energy per unit length is E = U × I × 60 / (v × 1000) in kJ/mm, with travel speed v in mm/min. Only part of it enters the plate, so the effective heat input is Q = η × E. Ovako lists the thermal efficiency η as 0.8 for MMA and MIG/MAG, 0.6 for TIG and plasma, and 1.0 for submerged arc welding, together with typical effective heat inputs that make a handy sanity check:

Thermal efficiency and typical effective heat input (Ovako welding guide)
ProcessηTypical Q (kJ/mm)
MMA / SMAW0.81–4
MIG/MAG / GMAW0.80.5–3
TIG / GTAW and plasma0.60.5–2.5
Submerged arc / SAW1.02–6

If you are comparing processes, our metallurgy guides to GMAW (MIG) and submerged arc welding cover how each one loads the joint with heat.

Watch the shape factor. F belongs inside the t8/5 equation, not in the heat input. Multiplying it into Q as well counts it twice.

Should I use the 2D or the 3D equation? Transition thickness

Whether a plate behaves as thin or thick is not fixed by the plate alone. It depends on how much heat you put in and on the preheat. The dividing line is the transition thickness dt, the thickness at which the two equations give the same t8/5. Setting them equal and solving for d gives:

d_t = sqrt( [(4300 − 4.3·T0) · 10^5 / (6700 − 5·T0)] · Q · [ (1/(500−T0)^2 − 1/(800−T0)^2) / (1/(500−T0) − 1/(800−T0)) ] · F2/F3 )

If d is below dt, the 2D equation governs. If d is above it, the 3D equation governs. Because the thin-plate value is the longer one for thin plate and the thick-plate value is the longer one for thick plate, taking the greater of the two always gives the same answer, which is what Auto mode does.

How to choose between the 2D and 3D t8/5 equation Flowchart: compute net heat input, compute both the 2D and 3D cooling times, then take the greater value. If plate thickness is below the transition thickness the 2D value governs, otherwise the 3D value governs. 1. Net heat inputQ = η × U × I × 60 / (v × 1000) kJ/mm 2. Compute t2D and t3Dusing T0, d, F2, F3 and Q 3. Transition thickness d_tthe thickness where t2D = t3D Is d < d_t ?(same as t2D > t3D) YesNo 2D (thin plate)t8/5 = t2D 3D (thick plate)t8/5 = t3D
Choosing between the 2D and 3D equation. Comparing the two results is equivalent to comparing d with dt.

Because dt rises with heat input, the same 12 mm plate can behave as thin plate at high heat input and as thick plate at low heat input. Table 2 below shows how far that threshold moves.

Which joint shape factor should I use?

The shape factors describe how many directions heat can escape in. An open bead on plate loses heat in every direction. A fillet in a T-joint has more steel around it, so it cools faster and its factor is lower. Ovako’s table of the EN 1011-2 factors:

Joint shape factors
Joint typeF2 (2D)F3 (3D)
Run on plate1.01.0
Between runs in butt welds0.90.9
Single-run fillet weld, corner joint0.67 to 0.90.67
Single-run fillet weld, T-joint0.45 to 0.670.67

Where F2 is a range, the calculator shows the result at both ends so you can see the spread rather than a falsely precise single number.

Worked examples

Example 1: thick plate, 3D heat flow

MAG welding (η = 0.8) at 250 A, 26 V and 300 mm/min on 40 mm plate, a run on plate (F = 1.0), no preheat (T0 = 20 °C).

  1. Arc energy: E = 250 × 26 × 60 / (300 × 1000) = 1.30 kJ/mm. Net heat input: Q = 0.8 × 1.30 = 1.04 kJ/mm.
  2. 3D: (6700 − 100) × 1.04 × (1/480 − 1/780) = 6600 × 1.04 × 0.00080128 = 5.5 s.
  3. 2D for comparison: 0.77 s, and the transition thickness is 14.9 mm. The plate is thicker than that, so 3D governs: t8/5 ≈ 5.5 s.

That is at the short end of the range usually quoted for high-strength structural steels, so a steel with high hardenability would call for preheat or more heat input.

Example 2: thin plate, 2D heat flow

The same arc settings on 8 mm plate, run between runs in a butt weld (F2 = F3 = 0.9), T0 = 20 °C, so Q is still 1.04 kJ/mm.

  1. 2D: (4300 − 86) × 105 × (1.04/8)2 × (1/4802 − 1/7802) × 0.9 = 17.3 s.
  2. 3D for comparison: 5.0 s. The transition thickness is 14.9 mm, and 8 mm is below it, so 2D governs: t8/5 ≈ 17.3 s.

The thinner plate cools much more slowly for the same heat input, because the heat cannot spread through the thickness. The calculator reproduces both results exactly.

How do heat input and preheat change t8/5?

The tables below are computed from the equations above for a thick plate on a run on plate (F3 = 1.0). For other joint types multiply Table 1 by F3, for example 0.9 for runs in a butt weld.

Table 1. 3D t8/5 in seconds, by net heat input (rows, kJ/mm) and preheat (columns, °C)
Q (kJ/mm)20 °C100 °C150 °C200 °C250 °C
0.52.63.33.94.85.9
1.05.36.67.89.511.9
1.57.910.011.814.317.8
2.010.613.315.719.023.8
2.513.216.619.623.829.7
3.015.919.923.528.535.7
Table 2. Transition thickness dt in mm (plates thicker than this follow the 3D equation)
Q (kJ/mm)20 °C100 °C150 °C200 °C250 °C
0.51011121213
1.01516161719
1.51819202123
2.02122232526
2.52325262729
3.02527283032

Moving from 20 °C to 200 °C raises the 3D cooling time by a factor of about 1.8 at any heat input. That is why preheat is the standard lever for slowing cooling. Ovako’s guidance is to use preheating and a raised working temperature rather than more heat input to avoid hard, brittle structures, because excessive heat input reduces impact toughness through grain growth. For sizing the preheat itself, use our welding preheat temperature calculator and the guide to preheat and interpass temperature.

What t8/5 should I aim for?

There is no single correct number. For high-strength structural steels, Ovako recommends roughly 5–25 s, which corresponds to about 1–2 kJ/mm effective heat input, and notes that a time that is too short raises the risk of cold cracking while one that is too long lowers impact toughness. Steel producers publish narrower, grade-specific windows for higher-strength plate. Use those, and treat the calculator as a way to find parameters that land inside them.

Because the HAZ microstructure and its hardness are linked, procedure trials normally check hardness too. Ovako states that a HAZ hardness under 350 HV usually causes no problem, with about 400 HV acceptable when very low-hydrogen consumables are used and about 450 HV when an increased working temperature is applied. Our overview of hardness testing methods explains how those readings are taken.

Common mistakes and limits of the calculation

  • Wrong speed units. Travel speed must be in mm/min. Entering mm/s makes the heat input 60 times too small.
  • Arc energy mistaken for heat input. E is not Q. Multiply by the thermal efficiency η first.
  • Shape factor applied twice. F goes in the t8/5 equation only.
  • Using one equation without checking. Compare 2D and 3D, or use Auto mode.
  • Wrong working temperature. T0 is the temperature at the start of that pass: the preheat for the first run and the actual interpass temperature for later runs.
  • Wrong material. The equations are given for C-Mn and low-alloy steels. Do not use them for stainless, quenched-and-tempered or creep-resistant grades without material-specific guidance.
  • Treating the result as exact. It is an estimate. Complex joints, multi-pass build-up and welding position all move the real value, so confirm important procedures with thermocouple measurements on a test weld and qualify them under the applicable procedure standard, for example EN ISO 15609-1 or ASME IX.
Check the calculator against known cases

Set Heat input source to “Enter net heat input Q”, joint type to Custom, and compare with these independently calculated results.

Q (kJ/mm)T0 (°C)d (mm)F2 = F3t8/5 (s)Regime
1.220501.06.353D
1.02061.031.572D
1.5150200.910.732D (near the transition)
2.5200701.023.753D

Frequently asked questions

What is t8/5 and why is the 800–500 °C range used?

t8/5 is the time, in seconds, that the heat-affected zone takes to cool from 800 °C to 500 °C after a weld pass. In most structural steels this is the temperature range in which austenite decomposes into ferrite, pearlite, bainite or martensite, so the time spent in it largely decides the HAZ microstructure and hardness.

Which equation applies, 2D or 3D?

Compute both. The thin-plate (2D) value is the longer one when the plate is thinner than the transition thickness, and the thick-plate (3D) value is the longer one when it is thicker. The valid result is the greater of the two, which is the same as using 2D below the transition thickness and 3D above it. The calculator does this automatically in Auto mode.

How much does preheat change t8/5?

A lot. For a thick plate (3D) the same heat input gives about 1.8 times longer t8/5 at 200 °C than at 20 °C in the worked tables on this page. This is why raising the working temperature is the usual way to slow cooling without increasing heat input, which can reduce toughness.

What t8/5 should I aim for?

It depends on the steel grade. Ovako’s welding guide suggests about 5–25 s, roughly 1–2 kJ/mm effective heat input, for high-strength structural steels, noting that too short a time raises cold-cracking risk and too long a time lowers impact toughness. Steel producers publish grade-specific windows, and the qualified welding procedure always governs.

Can I use these equations for stainless steel, quenched and tempered or Cr-Mo steels?

No. The EN 1011-2 equations as used here are given for C-Mn and low-alloy steels. Other materials need material-specific guidance from the producer or the applicable application standard, and the result should be checked by measurement on a test weld.

Standards and references

  1. EN 1011-2:2001, Welding. Recommendations for welding of metallic materials. Arc welding of ferritic steels. CEN. Source of the cooling-time equations and joint factors.
  2. Ovako, Welding Guide (document CO-92 GB 19:11, 2019), sections 3.1 to 3.4 and 8.3. Steelmaker guidance on cooling time, thermal efficiency, joint factors and hardness limits. Available from ovako.com.
  3. EN ISO 15609-1, Specification and qualification of welding procedures for metallic materials. Welding procedure specification. Arc welding.
  4. Further reading: K. Easterling, Introduction to the Physical Metallurgy of Welding, 2nd ed., Butterworth-Heinemann; S. Kou, Welding Metallurgy, 2nd ed., Wiley.

Related reading

Riyanshi

← Previous
Fatigue Life Calculator (S-N Curve Based)
Next →
Controlled Rolling of Steel Plate